Brønsted acid site concentration: a key parameter for the synthesis of Zeolite-Templated Carbons
Year: 2022
Type: conference-paper
Abstract: INTRODUCTIONZeolite-templated carbons (ZTCs) have been synthesized for the first time by Kyotani (1997) and are today a well-established class of microporous carbons. They feature defined textural proprieties that reveal very interesting in a number of fields including (electro)catalysis and adsorption as shown by Wang (2009), due to their unique electronic properties in combination with very high porous volume and homogeneous micropore size distribution related in Nishihara’s review (2018). These ZTCs develop within the microporous system of a template zeolite and are hence a negative copy of their structure.In this communication, we present the impact of the active site concentration of the template zeolite (FAU structure) and the synthesis temperature on the properties of achieved ZTCs. Despite the known impact of acid site density in many zeolite catalyzed reactions, this parameter has never been taken into consideration for ZTC synthesis. The thorough characterization of hybrid materials (zeolites/carbon) and final ZTCs by nitrogen physisorption, XRD, electron microscopy, conductivity, MAS NMR, Raman, and EPR allowed us to draw sound conclusions on the ZTC formation mechanism as a function of the studied parameters.MATERIALS AND METHODSFive proton-exchanged FAU structured zeolites with acidities varying from 54 to 1004 μmol g-1 were used as zeolite templates. After activation of the zeolites, ethylene flow (6.7vol% in N2) was passed through at a target temperature (690, 740, 790, and 840 °C) for 4 h. Additional pyrolysis treatment was carried out at 900 °C for 2 h under N2 flow. The achieved hybrid materials were treated with aqueous HF, which allowed to dissolve the template zeolites and obtain the pure ZTCs.RESULTS AND DISCUSSIONIn a relatively narrow range of synthesis temperatures very different behaviors of ZTCs formation can be identified. For low synthesis temperatures (i.e. 690 and 740 °C), the structural packing density (SPD) of the hybrid materials which refers to the amount of carbon within the zeolite micropores, clearly depends on the acidity. By increasing the acidity, an increase in SPD can be noted as well as a decrease of the residual microporous volume of the hybrid material. That informs about carbon filling within the micropores only, where the acid sites are located. For a synthesis temperature of 790 °C, a similar SPD no matter the acidity of the template zeolite is obtained as well as an almost complete filling of micropores. On the contrary, using the highest synthesis temperature (840 °C) involves a decrease of the SPD by increasing the acid site content. This can be explained by the textural properties of the template zeolites: mesoporous volume that is filled usingthis temperature decreases linearly by lowering Si/Al ratio. Acid sites no longer govern the synthesis of ZTC but it is the textural properties of the template zeolite.These observations are confirmed by characterizing the final ZTC materials after zeolite dissolution. TEM images show perfect replicas of zeolite for low synthesis temperatures only when the acid site content is high enough. On the contrary, when a zeolite containing low acidity is used as template a mixture of ZTC and unstructured carbon compound is obtained. At 790 °C, the morphology of the ZTC is similar to the one of the template zeolite no matter the acidity of the template. Finally, at 840 °C the morphology is also transcribed to the ZTC but external carbon deposition occurs as well as mesopore filling. The composition also depends both on the synthesis temperature and acid sites content: using low synthesis temperature C/H ratios clearly decrease by decreasing the acidity while these ratios are equal no matter the acidity at 790 °C, and increase by decreasing the acidity at 840 °C due to mesopores filling and carbon deposition on the external surface.Interestingly, ZTC which seemed to present similar properties for a synthesis temperature of 790 °C show important differences as far as their electronical conductivity, as well as their structuring order are concerned. This can be explained by a higher amount of acid sites that favor condensation of carbon compoundsCONCLUSIONSThese observations together with nitrogen physisorption, electron microscopy images, Raman, and EPR spectroscopy allow to conclude that as a function of the acid site concentration and synthesis temperature different ZTC formation mechanisms are involved: the synthesis of ZTCs i) using low and medium synthesis temperatures (i.e. 690, 740 and 790 °C) the synthesis is importantly impacted by the acid site concentration. and, ii) using high synthesis temperature (i.e. 840 °C) the textural properties of the zeolite sole seem to direct the synthesis of carbons.AcknowledgmentsThe authors acknowledge financial support from the European Union (ERDF) and “Région Nouvelle Aquitaine”.ReferencesKyotani, T., Nagai, T., Inoue, S., Tomita, A. (1997). Formation of New Type of Porous Carbon by Carbonization in Zeolite Nanochannels. Chem. Mater., 9, 609-615. https://doi.org/10.1021/cm960430hNishihara, H., Kyotani, T. (2018). Zeolite-templated carbons – three-dimensional microporous graphene frameworks. Chem. Commun., 54, 5648-5673. https://doi.org/10.1039/C8CC01932KWang, H. L., Gao, Q. M., Hu, J., Chen, Z. (2009). High performance of nanoporous carbon in cryogenic hydrogen storage and electrochemical capacitance. Carbon, 47, 2259-2268. https://doi.org/10.1016/j.carbon.2009.04.021
Source: HAL
Language: English
Subfield: Inorganic Chemistry
Field: Chemistry
Domain: Physical Sciences
Open Access status: green
OpenAlex ID: W4407803586