Year: 1976
Type: report
Abstract: Small-scale production and mechanical properties of TATB/Kel-F 800 (92.5/7.5), a useful plastic bonded explosive, are described. TATB particles are slurried in water while adding a solvent solution of Kel-F. As the solvent is removed from the slurry at 75 to 80/sup 0/C under vacuum, the fine particles of TATB become coated with Kel-F and clump together to form granules. After drying at 80/sup 0/C the granules are pressed at 120/sup 0/C and 138 MPa (20,000 psi) to form needed shapes.
DOI: 10.2172/7193237
Author: J. S. Hallam
Language: English
Subfield: Materials Chemistry
Field: Materials Science
Domain: Physical Sciences
Open Access status: green
OpenAlex ID: W64375596