Experimental and Numerical Simulation Study on the Load-Carrying Capacity of PCCP with Broken Wires Repaired by the Internal Steel-Cylinder Method
Year: 2026
Type: article
Abstract: Objective Prestressed concrete cylinder pipes (PCCPs) are widely used in water-diversion and water-supply systems. Their structural performance depends on the interaction of the concrete core, embedded steel cylinder, mortar coating, and circumferential prestressing wires. During service, corrosion, material deterioration, construction defects, and pressure fluctuations may cause wire breakage. The resulting local prestress loss can promote cracking, relative movement between the wires and concrete, and stress concentration in the original steel cylinder. Internal steel-cylinder repair is a promising method, but the load-transfer mechanism between the strengthening cylinder, grouting layer, and original pipe requires further clarification. This study investigates the mechanical response and damage evolution of a PCCP with local wire breakage before and after repair. The objectives are to characterize component responses under internal pressure, quantify the strain-reduction effect of repair, and examine the coordinated action of the strengthening cylinder and grouting layer.Methods A full-scale PCCP-E specimen was tested under internal water pressure. The pipe was 6 000 mm long with an inner diameter of 1 600 mm. The concrete core was 110 mm thick; the embedded impermeable steel cylinder was 1.5 mm thick; the prestressing wires had a diameter of 5.0 mm, a spacing of 35.5 mm, and a nominal tensile strength of 1 540 MPa; and the outer mortar coating was 45 mm thick. Six measurement windows were arranged on the north and south sides at axial positions of 1 500, 3 000, and 4 500 mm. Strain gauges were installed on the concrete core, prestressing wires, and mortar coating, and an optical-fiber sensor was used at one selected window.Results and Discussions For the intact pipe, the first visible cracks appeared in the pipe-end socket region at approximately 0.6 MPa. At approximately 1.0 MPa, intermittent cracking sounds and local relative movement between the prestressing wires and concrete core were observed. Existing cracks extended as the pressure approached 1.2 MPa, and the first-stage loading was stopped for safety. The pipe-end region was more sensitive to local damage because of geometric discontinuity and boundary effects.Conclusions The full-scale test and finite-element analysis show that local wire breakage weakens circumferential restraint and promotes damage concentration near the broken-wire region and pipe-end socket. Under the investigated monotonic internal-pressure conditions, internal steel-cylinder repair reduced the response of the original pipe and improved deformation compatibility. The strengthening cylinder and grouting layer formed an internal support system, with the grouting layer providing continuous radial compression transfer under the adopted dense-grouting and tied-interface assumptions. The reported reductions apply to the tested pipe geometry, the approximately 5% nominal local wire-breakage arrangement, the adopted repair configuration, and the investigated pressure range. Because the full-scale test ended at 1.6 MPa and did not include ultimate failure, the results should be interpreted as pressure-response and repair-effectiveness evidence rather than an ultimate load capacity. Future studies should consider different wire-breakage distributions, grouting defects and interface slip, external soil and traffic loads, cyclic and transient pressures, and long-term corrosion and prestress loss.
Source: 工程科学与技术
Language: Chinese
Subfield: Building and Construction
Field: Engineering
Domain: Physical Sciences
Open Access status: diamond
OpenAlex ID: W7204152605