Year: 2025
Type: article
Abstract: The properties of carbon nanotubes and their applications are still being studied. In recent years, the production of carbon nanotubes (CNT) has been carried out by three different techniques: arc discharge between two graphite electrodes [1-5] chemical vapor deposition (CVD) [6-10] and; Laser ablation [11-13]. Both laser ablation and arc discharge produce high-quality SWNT. Among the methods presented, CVD is the most adaptable method for large-scale CNT production at a lower cost [6]. In the CVD method, the first role of the catalyst is to decompose the hydrocarbon molecules and then promote the formation of CNT [14, 15]. The control of the production, selectivity and quality of CNT comes from the combination of the properties of the catalysts and the real parameters. Thus, this project aims to synthesize and investigate new catalysts for the production of carbon nanotubes, mainly SWNT, by the CVD method. Recently, the introduction of new strategies has customized the production of CNTs. A recent study shows how the use of a monocrystalline silicon substrate causes single-walled carbon nanotubes (SWCNTs) to grow in an oriented manner, nanotubes with lengths of up to 18.5 cm [16]. The helical or spring-like morphology of CNTs has aroused great interest in the scientific field [17]. The starting material used to obtain the supports is alumina Al2O3 (Puralox). The supports were heated in a muffle furnace to 550°C at a rate of 10°C/min. The iron catalyst was prepared by dry impregnation on the alumina substrate in a proportion of 5% by weight. Iron nitrate nonahydrate Fe(NO3)3 9H2O was used as the metal precursor. After the impregnation step, the sample was subjected to a drying step aiming at the elimination of the solvent. This drying will be done in an oven at 120°C for approximately 12h. The catalyst calcination step was performed in a muffle furnace, in the presence of air. The calculation of the specific area, pore volume and average pore diameter of the iron catalyst were obtained from the measurement of the adsorption of an inert gas, N2, on the surface of the catalyst. The analyses were performed in a Micromeritics ASAP 2020 apparatus. The experimental procedure included drying the samples in an oven at 120°C for 12 hours. The sample was then placed in the ASAP unit reactor. The pretreatment step was carried out at 200°C for 6 hours, under vacuum, to remove any moisture that may exist in the sample. After the pretreatment step, the reactor was transferred to the analysis section of the equipment. The test was conducted at a cryogenic temperature, using liquid nitrogen at 1 atm. The specific area was calculated using the BET (Brunauer-Emmett-Teller) methodology and the total pore volume and pore diameter distribution were done using the BJH (Barrett-Joyner-Halenda) method. Specific area: 178 m2/g , pore volume and average: 0.44 cm3/g and pore diameter: 6,9 nm were the results. X-ray diffraction (XRD) analyses allowed the identification of the crystalline phases of the supports and the iron catalyst. The analyses were performed in a Rigaku Miniflex model equipment, using CuKα radiation (1.540 Å). The diffractograms will be obtained using the range 2θ: 10-100°, step of 0.02° and a scanning speed of 1° per min. After the diffractograms were produced, they were compared with crystallographic charts to verify the phases present. The diffractogram of the catalyst of the Fig. 1 shows the presence of the γ-Al2O3 and iron oxide Fe2O3 (hematite) peaks. For observation under the transmission electron microscope, this same sample of catalyst powder was dispersed in isopropyl alcohol and dripped onto a copper grid with a holey carbon film. A JEM 2100F transmission electron microscope from LabNano-CBPF (Brazilian Center for Physics Research) operating at 200 kV was used. Large alumina particles of the order of hundreds of nm to microns with a clear contrast and iron oxide particles of the order of 20 nm with a dark contrast were observed impregnated on the surface of the matrix, homogeneously dispersed (Fig. 2a). Based on the XRD results, it was determined that these dark particles are hematite (α-Fe2O3). In Fig. 2b, it can be seen that the hematite particles have an undefined morphology and a more heterogeneous size dispersion than in the other region of the sample. A methane flow over catalysts was used as the carbon source for the production of CNTs. The method for producing carbon nanotubes was chemical vapor deposition. A module containing a quartz reactor, furnace, and flow and temperature control systems was used, as well as connections to the N2, CH4, and H2 gas supply lines. The method consists of placing 0.5 g of catalyst inside a vessel inside a 2.5 cm diameter quartz tube that is positioned vertically. The tube is heated by a tubular furnace to a temperature of 600°C at a rate of 10°C/min while H2 flows inside the tube. Once 600°C was reached, the H2 flow was exchanged for methane, initiating the formation of CNTs. The reaction time was 30 min and the entire process was carried out at atmospheric pressure. The morphological analysis of the carbon nanotubes obtained was performed using a Fei Tecnai Spirit transmission electron microscope at 120 kV. The sample preparation follows the same procedure descripted previously for the catalyst sample. The Fig. 3 shows the presence of carbon nanotubes with spring morphology. The image of the Fig. 4 was assembled from four images in sequence and it is possible to observe the nano spring structure with more details. The nano spring structure is a result from a coiled nanotube with a 30-40 nm external, 6-8 inner diameter, ∼12mm wall thickness and ∼1 µm length. This formation mechanism probably occurred due to a high nucleation rate and low growth rate during the synthesis process, promoting the formation of growth nuclei stacked with each other at a preferential angle forming the helical structure [18]. XRD diffractogram of the catalyst 5% Fe supported in alumina (5%Fe/Al2O3). Multi-beam TEM micrographs: (a) porous alumina matrix with iron particles impregnated on its surface, (b) detail of iron oxide (Fe2O3) particles of the order of 20 nm. Multibeam TEM micrography of CNTs whit helicoidal morphology. Multi beam TEM image of carbon nano spring (detail of the Carbon Nano Springs marked in the yellow frame on the Fig. 3).
Source: Microscopy and Microanalysis
Language: English
Subfield: Materials Chemistry
Field: Materials Science
Domain: Physical Sciences
Open Access status: bronze
OpenAlex ID: W4412909752